To constantly improve the management system by virtue of the rule of "sincerely, good faith and quality are the base of enterprise development", we widely absorb the essence of related products internationally, and constantly develop new products to meet the demands of customers for 11 Years Manufacturer Titanium alloy 10V-2Fe-3Al UNS R56410 to Guatemala Factory, We will wholeheartedly welcome all clients in the industry both at home and abroad to cooperate hand in hand, and create a bright future together.
HY Titanium 10-2-3 Material grades and equivalents
10-2-3 Titanium, UNS R56410
Introduction
HY Titanium 10-2-3 is a near beta alloy developed as a high strength forging alloy. This grade provides the best combination of strength and toughness of the commercially available titanium alloys. Its strength permits about a 27% weight savings when compared to Ti-6Al-4V. At the 180 ksi tensile strength level, the K1cvalue is 40 ksi-in ½ minimum. Solution treated and aged material possesses excellent resistance to stress corrosion cracking, typically K1scc being greater than 0.8 K1c. Solution treated material should not be subject to long term exposure in the 500-800°F range. This could result in high strength but low ductility.
High strength condition: Solution treat 60-100°F below the beta transus (typically 1460-1480°F), not less than 30 minutes, water quench. Age 900-975°F not less than 8 hours, air cool. For lower strength, overage in the 950-1150°F range. This alloy is deep hardenable, capable of high strengths in sections up to approximately 4″ thick.
This grade is usually supplied as billet or bar, finish rolled or forged in the alpha-beta field. For the high strength condition, the forging is usually given a pre-form forge above the beta transus, followed by 15-25% reduction below the beta transus.
Chemistry Composition
|
V |
Al |
Fe |
C |
N |
O |
H |
Y |
Others, |
Others, |
Ti |
MIN |
9.0 |
2.6 |
1.6 |
- |
- |
- |
- |
- |
- |
- |
- |
MAX |
11.0 |
3.4 |
2.22 |
0.05 |
0.05 |
0.13 |
0.015 |
0.005 |
0.10 |
0.30 |
Balance |
Features
- High strength and toughness
- Weight savings when compared to Ti-6Al-4V
- Excellent resistance to stress corrosion cracking
Applications
- Hand and die forgings
- Aircraft landing gear
- Golf club driver faces
Physical Properties
Density: 0.168 lb/inch³
Nominal Beta Transus: 1470°F
Poisson’s ratio: 0.32
Thermal Expansion: 75-800°F, 5.4×10-6 in/in°F
Tensile Modulus: 15.9×106 psi
Modulus: 16.2×106 psi
* 70°F to indicated temperature.
Mechanical Properties
Minimum Mechanical Properties AMS 4984, solution treated and aged
Ultimate Tensile Strength, ksi |
173 |
Ultimate Tensile Strength, ksi |
160 |
0.2% Yield Strength, ksi |
4 |
Reduction of Area, % |
Report |
fracture toughness, k1C |
40 ksi |
AMS 4987, single solution heat treat & overage
Ultimate Tensile Strength, ksi |
140 |
0.2% Yield Strength, ksi |
130 |
Elongation, % |
8 |
Reduction of Area, % |
20 |
fracture toughness, k1C |
80 ksi |
Regular shape for all kinds of alloys | |||
Form | Specification | Supply Form | Others |
Sheet | Thickness:0.40-4.75mm,General Width:1000、1219、1500mm | Whole Coil or piece of it | Cold Annealed,Surface 2B、2E |
Plate | Thickness:4.76-60mm,Width:1500、2000、2500mm,Length:3000、6000、8000、8500mm(Under 10mm plate can be coiled) | Whole Coil or piece of it | Single hot rolling,Solid solution annealed state,Surface 1D |
Belt | Thickness:0.10-3.0mm,Width:50-500mm | Whole Coil or Specified size | Cold Annealed,Surface 2B、2E |
Bar & Rod | Rolled barΦ5-45mm,Length≤1500mm | Polished Bar(circle、Square) | Solution annealing,descaling |
Forged barΦ26-245mm,Length≤4000mm | |||
Weld tube | Outer diameterΦ4.76-135mm,Wall Thickness0.25-4.00mm,Length:≤35000 mm | Base on your requirement | |
Seamless Tube | Outer diameterΦ3-114mm,Wall Thickness0.2-4.5mm | Base on your requirement | |
Wire | Outer diameterΦ0.1-13mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
Forged piece | discs,rings,squares,blocks,slabs | Base on your requirement | Steel, Alloy |
Flangs | All kinds of Flangs | Base on your requirement | Steel, Alloy |
Welding Material | Coil wire Φ0.025mm-1.6mm | Base on your requirement | Certificate of Origin:America, Sweden, Britain, Germany, Austria, Italy, France. |
Straight WireΦ1.6mm-4.0mm | |||
Welding rodΦ1.2mm-4.0mm | |||
Tube | Elbow, three links, four links, different diameter size | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
Explosive bonded laminate | Raw Sheet Thickness≥2mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
This is our 4000 watt Co2 laser slicing process. We can cut Stainless Steel and alloys to .five hundred”, Steel and metal alloys to .750″ and aluminum to .375″. Equally our devices have big bed dimensions, just one is sixty” x 120″ and the 3000 watt is seventy eight” x 157″. Equally devices have automatic loading and shuttle tables for prototyping to manufacturing.
Melting down 1 gram bars of Silver, Copper, Nickel and Brass with hydrogen and oxygen. Brass is previously an alloy of copper and zinc, and did not soften down effortless as a I figured out from my Brass, Guide and Gunpowder video clip. I then blend the a few workable metals Silver, copper and nickel to generate…….Silvcopickel
SUBSCRIBE: http://comprehensive.sc/1bnslc9
Facebook: http://comprehensive.sc/1dT2aaM
RHNB Vs. Watermelon – http://comprehensive.sc/1bns60F
RHNB Vs. Jello – http://comprehensive.s/1bns0WF RHNB Vs. Elmers Glue – http://comprehensive.sc/1dT1TEM
RHNB Entire Playlist – http://comprehensive.sc/1dT1WjP -Want to ship an object / materials / substance to be RHNB’d or HHO’d? Send Here with a comprehensive credit of your donation! PO Box 21 96 Seymour St. Tonawanda NY 14150 Usa