To be the stage of realizing dreams of our employees! To build a happier, more united and more professional team! To reach a mutual benefit of our customers, suppliers, the society and ourselves for Special Price for Titanium alloy 6Al-4V ELI UNS R56401 Manufacturer in Kazakhstan, As we are moving forward, we keep an eye on our ever-expanding product range and make improvement to our services.
HY Titanium 6-4 ELI Material grades and equivalents
6-4 ELI Titanium, 6-4 ELI, UNS R56401
Introduction
Low interstitial version of HY Titanium 6-4 ELI, for maximum toughness. Preferred for marine and cryogenic applications. This grade is normally used in the annealed condition. HY Titanium 6-4 ELI is the preferred choice for the medical implant field.
Stress relief 900-1200°F 1 to 4 hours, air cool. Duplex anneal, bar and forgings: Solution anneal 50-100°F below the beta transus, hold 1 hour minimum, air cool. Then reheat within the range 1300-1400°F, hold 1 hour minimum, air cool. Stress – relief annealing is performed after welding.
Chemistry Composition
Al |
V |
Fe |
O |
C |
N |
H |
Y |
Others, |
Others, |
Ti |
|
MIN |
5.5 |
3.5 |
– |
– |
– |
– |
– |
– |
– |
– |
– |
MAX |
6.5 |
4.5 |
0.25 |
0.13 |
0.08 |
0.03 |
0.0125 |
0.005 |
0.1 |
0.4 |
Balance |
Features
Resistant to bodily fluidsResistant to a variety of corrosive environmentsFreedom from chloride stress corrosion crackingGood strength and toughness over a wide temperature rangeHigh resistance to erosion corrosion and corrosion fatigueUseful resistance to dry chlorine, fluorine, hydrogen chloride and hydrogen fluoride gases
Applications
Medical and dental implantsCryogenicsAerospaceChemical processing
Physical Properties
Density: 0.160 lb/in3
Melting Range: 2370 – 2460°F
Beta Transus: 91790+25°F
Minimum Tensile Properties, AMS 4919, Duplex Annealed
Temperature, °F |
68-212 |
68-600 |
68-1000 |
68-1200 |
68-1500 |
Coefficient* of Thermal Expansion, in/in°F x 10-6 |
9.18 |
9.54 |
10.08 |
10.44 |
10.8 |
Mechanical Properties
Typical hardness Rockwell: C 30-34 Specific minimums, AMS 4931, bar and forging
Representative Tensile Properties, Sheet
Diameter, in |
< 3.0 |
< 3.0 < 4.0 |
< 4.0) < 6.0 |
Tensile Strength, ksi |
125 |
123 |
120 |
0.2 % Yield Strength, ksi |
115 |
110 |
110 |
Elongation, % *L (**ST) |
10 (8) |
10 (8) |
8 (8) |
Reduction of Area, % *L (**ST) |
25 (–) |
20 (15) |
15 (15) |
* Longitudinal ** Short Transverse
Typical Elevated temperature Properties
Temperature, °F |
93 (200) |
149 (300) |
204 (400) |
260 (500) |
Ultimate Tensile Strength, ksi |
843.3 (121) |
772.2 (112) |
723.9 (105) |
657.7 (98) |
0.2 % Yield Strength, ksi |
710.2 (103) |
641.2 (93) |
586.1 (85) |
531.0 (77) |
Elongation, % |
13 |
15 |
16 |
16 |
Regular shape for all kinds of alloys | |||
Form | Specification | Supply Form | Others |
Sheet | Thickness:0.40-4.75mm,General Width:1000、1219、1500mm | Whole Coil or piece of it | Cold Annealed,Surface 2B、2E |
Plate | Thickness:4.76-60mm,Width:1500、2000、2500mm,Length:3000、6000、8000、8500mm(Under 10mm plate can be coiled) | Whole Coil or piece of it | Single hot rolling,Solid solution annealed state,Surface 1D |
Belt | Thickness:0.10-3.0mm,Width:50-500mm | Whole Coil or Specified size | Cold Annealed,Surface 2B、2E |
Bar & Rod | Rolled barΦ5-45mm,Length≤1500mm | Polished Bar(circle、Square) | Solution annealing,descaling |
Forged barΦ26-245mm,Length≤4000mm | |||
Weld tube | Outer diameterΦ4.76-135mm,Wall Thickness0.25-4.00mm,Length:≤35000 mm | Base on your requirement | |
Seamless Tube | Outer diameterΦ3-114mm,Wall Thickness0.2-4.5mm | Base on your requirement | |
Wire | Outer diameterΦ0.1-13mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
Forged piece | discs,rings,squares,blocks,slabs | Base on your requirement | Steel, Alloy |
Flangs | All kinds of Flangs | Base on your requirement | Steel, Alloy |
Welding Material | Coil wire Φ0.025mm-1.6mm | Base on your requirement | Certificate of Origin:America, Sweden, Britain, Germany, Austria, Italy, France. |
Straight WireΦ1.6mm-4.0mm | |||
Welding rodΦ1.2mm-4.0mm | |||
Tube | Elbow, three links, four links, different diameter size | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
Explosive bonded laminate | Raw Sheet Thickness≥2mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
http://www.weldingtipsandtricks.com/metals-and-how-to-weld-nickel.html
How to weld nickel alloys like hastelloy, inconel, etc. Nickel alloys have a low thermal conductivity and so limiting heat input and using lower amperage than would be used for stainless is one key to making good nickel alloy welds.
Riporto(placcatura)con filo Nimonic 80 dia. one.2 eseguito con inverter multiprocesso Weldtronic Synertech 8004 Digit in pulsato sinergico.
NB .Il lampeggio dell’arco è presente solo nella ripresa effettuata dalla fotocamera digitale usata probabilmente a causa di interferenza con l’intenso arco luminoso.
Details: belda1@tiscali.it